Researchers in China have investigated how screen printing of photoresist degrades copper-plated silicon heterojunction (HJT) solar cells and have proposed a modified screen design intended to limit that damage. The findings, published in Solar Energy, pair a diagnosis of the wear mechanism with a mitigation experiment on screen geometry.
Screen printing is a standard step in solar cell metallization, and copper plating is being pursued as a way to cut metallization costs and reduce reliance on silver. The mechanical pressure and thermal treatments involved in printing can, however, damage the sensitive passivating contact structures of HJT cells, raising recombination losses and lowering conversion efficiency.
A different contact regime from silver paste
Corresponding author Lang Zhou told pv magazine that photoresist printing in HJT production works on different terms from conventional silver paste printing. In silver paste printing, the screen openings cover only 2–5% of the total area, and the remaining surface carries an emulsion layer that keeps the mesh from touching the wafer directly. Full-area photoresist coating, by contrast, typically uses a screen without emulsion coverage so that resist is deposited evenly across the whole wafer, meaning the mesh comes into direct and extensive contact with the wafer on every printing cycle.
Earlier investigations cited by the researchers recorded a gradual efficiency decline from 26.2% to 25.7% across 15,000 consecutive printing cycles in commercial production. The losses were attributed mainly to reductions in open-circuit voltage and fill factor, while short-circuit current density and electrical resistance stayed largely unchanged. Minority carrier lifetime degradation rose from 0.61% with a new screen to 11.0% after 15,000 cycles.
Wear at the mesh knuckles
Using three-dimensional confocal microscopy, the team identified progressive wear of the screen mesh knuckles as the principal cause. As the knuckles wear down, their contact area with the wafer grows, placing greater mechanical stress on the passivation layers underneath. Scanning electron microscopy showed no visible surface scratches, but photoluminescence measurements confirmed higher recombination losses, pointing to damage at the sensitive amorphous silicon/crystalline silicon interface.
To counter this, the researchers developed an emulsion buffer layer intended to prevent direct contact between the mesh and the wafer surface. They evaluated six patterns with emulsion coverage ratios from 2.9% to 16.6%.
The trials revealed a trade-off between mechanical protection and photoresist coating uniformity: higher emulsion coverage reduced damage but impaired ink distribution. A coverage ratio of 4.7% gave the best balance, holding minority carrier lifetime degradation to 0.41% after 10,000 printing cycles while maintaining relatively good coating uniformity. The researchers attributed the improvement to the emulsion layer blocking direct mesh-to-wafer contact and thereby limiting cumulative mechanical damage to the passivation layers.
Zhou said the results show that a relatively simple change to screen design can substantially mitigate printing-induced degradation, offering a practical route to better manufacturing reliability for copper-plated HJT cells.
Broader push toward copper contacts
The study appears as copper metallization draws growing interest as a substitute for silver contacts in HJT devices. According to the account in the paper's press summary, researchers at China's Nankai University reported in April 2026 a silver-free HJT cell with 25.2% efficiency, combining plasma-induced interface engineering with copper electroplating and addressing adhesion, contact resistance and stability at the ITO interface. Separately, scientists at Germany's Forschungszentrum Jülich reached 23.08% efficiency in a fully copper-metallized HJT cell, a relatively small penalty compared with its silver-metallized counterpart, while cells pairing silver-copper paste on the front with silver contacts on the rear reached 23.95%. Both results point to copper's potential to reduce silver consumption, while leaving room for further gains in processing and electrical performance.